Open battery ageing data · UConn LFP
UConn LFP ageing data: 64 18650 cells under 11 cycling conditions
The UConn-ISU-ILCC LFP/graphite battery ageing dataset (Nowacki et al., Journal of Power Sources 2025) cycled 64 Lithium Werks APR18650M1B cells of 1.2 Ah in 11 groups. Each group has its own charge rate, discharge rate and depth of discharge (60, 80 or 100 %). About every 3.5 days a reference performance test measured each cell’s capacity, until the cells reached 80 % state of health. Lemonergy computed one row per cycle and one per reference test from the published files. The cycling rows are partial discharges, so only the reference tests are drawn. The CSV is large, so it is served gzip-compressed.
Download every row (CSV, gzip-compressed, 7.1 MB; 30.5 MB unpacked)Manifest (JSON): files, hashes, unitsChart and Excel downloadOriginal dataset
Free to download, no account needed. Or read it straight into Python:
import pandas as pd
cycles = pd.read_csv("https://lemonergy.com/data/ageing/uconn-reil-2025/cycles.csv.gz", compression="gzip")The CSV is 30.5 MB, over the 25 MiB a single file may have on this site, so it is served gzip-compressed (7.1 MB). Unpacked, it is byte for byte the file the manifest names: SHA-256 5b59a178ff4d72c5fc54735891003c31069a06e81a5f75ff4dd2d931cd7e2b75. The compressed file’s own SHA-256 is 7ac36f087be7dff51e26fa7a4cc1f0b1c061ab1cf81106421a79c612203609e2.
- Cells
- 64 cells, 18650; maker: LithiumWerks, as the dataset names it (contrib record cell/lithium-werks/apr18650m1b)
- Chemistry
- LFP/graphite (dataset title and README)
- Nominal capacity
- 1.2 Ah
- Rows
- 280,920, one row each
- Test programmes
- 11
- Published by
- University of Connecticut REIL / Iowa State University / Iowa Lakes Community College
- Licence
- CC BY 4.0
- Files retrieved
- 2026-11-11
Source: UConn-ISU-ILCC LFP/Gr Battery Aging Dataset, University of Connecticut REIL / Iowa State University / Iowa Lakes Community College. Licence: CC BY 4.0.
Cite: Nowacki, B., Ramamurthy, J., Thelen, A., Tischer, C., Pint, C. L., Hu, C. Rapid estimation of lithium-ion battery capacity and resistances from short duration current pulses. Journal of Power Sources 628, 235813 (2025). doi:10.1016/j.jpowsour.2024.235813
Licence and how to cite · Data quality · Every source file, by SHA-256
Capacity fade, cycle by cycle
Reference discharge capacity of each reference performance test, one coloured line per cell. The cycling rows are partial discharges and are not drawn. Point at a chart to read the values; download them as Excel.
The chart needs JavaScript; every cell’s values are in the table below and in the CSV.
Point at or touch a chart to read every cell’s value at that cycle. Drag across it with a mouse to zoom in. Click a line, or a cell’s name in the legend or table, to show that cell on its own; the others turn grey.Touch a chart to read the values at a cycle. Tap a cell’s name in the legend or the table to show it on its own; the others turn grey.
| Cell | Rows recorded | Points drawn | First (Ah) | Last (Ah) | Last / first |
|---|
Every cell
First and last discharge capacity of the rows the chart draws, for all 64 cells. Every row of every cell, with all its values, is in the CSV (gzip-compressed, 7.1 MB; 30.5 MB unpacked).
| Programme | Cell | Rows recorded | Points drawn | First (Ah) | Last (Ah) | Last / first |
|---|---|---|---|---|---|---|
| Group 1 | cell_02 | 3,739 | 35 | 1.213 | 0.959 | 79.1 % |
| Group 1 | cell_03 | 4,110 | 38 | 1.216 | 0.953 | 78.3 % |
| Group 1 | cell_04 | 3,823 | 36 | 1.211 | 0.956 | 79.0 % |
| Group 1 | cell_05 | 3,167 | 30 | 1.214 | 0.936 | 77.1 % |
| Group 1 | cell_06 | 3,853 | 36 | 1.208 | 0.951 | 78.7 % |
| Group 1 | cell_07 | 4,426 | 42 | 1.219 | 0.942 | 77.3 % |
| Group 2 | cell_08 | 4,693 | 41 | 1.212 | 0.955 | 78.8 % |
| Group 2 | cell_09 | 6,063 | 53 | 1.211 | 0.954 | 78.8 % |
| Group 2 | cell_10 | 4,059 | 36 | 1.217 | 0.954 | 78.4 % |
| Group 2 | cell_11 | 4,370 | 38 | 1.212 | 0.944 | 77.9 % |
| Group 2 | cell_12 | 4,943 | 44 | 1.214 | 0.949 | 78.2 % |
| Group 2 | cell_13 | 4,709 | 41 | 1.214 | 0.956 | 78.7 % |
| Group 3 | cell_14 | 2,595 | 23 | 1.214 | 0.940 | 77.5 % |
| Group 3 | cell_15 | 2,634 | 22 | 1.216 | 0.879 | 72.3 % |
| Group 3 | cell_16 | 2,673 | 22 | 1.213 | 0.890 | 73.3 % |
| Group 3 | cell_17 | 2,701 | 23 | 1.217 | 0.927 | 76.2 % |
| Group 3 | cell_18 | 2,730 | 23 | 1.211 | 0.931 | 76.9 % |
| Group 3 | cell_19 | 2,619 | 22 | 1.216 | 0.911 | 74.9 % |
| Group 4 | cell_20 | 4,764 | 61 | 1.215 | 0.948 | 78.0 % |
| Group 4 | cell_21 | 5,343 | 68 | 1.219 | 0.948 | 77.8 % |
| Group 4 | cell_22 | 4,949 | 63 | 1.213 | 0.955 | 78.8 % |
| Group 4 | cell_23 | 4,192 | 53 | 1.213 | 0.942 | 77.6 % |
| Group 4 | cell_24 | 4,256 | 54 | 1.216 | 0.949 | 78.0 % |
| Group 4 | cell_25 | 5,408 | 68 | 1.212 | 0.949 | 78.2 % |
| Group 5 | cell_26 | 7,002 | 58 | 1.214 | 0.959 | 79.0 % |
| Group 5 | cell_27 | 6,620 | 52 | 1.214 | 0.949 | 78.2 % |
| Group 5 | cell_28 | 6,556 | 54 | 1.216 | 0.960 | 78.9 % |
| Group 5 | cell_29 | 7,297 | 61 | 1.213 | 0.950 | 78.4 % |
| Group 5 | cell_30 | 6,867 | 57 | 1.215 | 0.959 | 78.9 % |
| Group 5 | cell_31 | 8,510 | 71 | 1.215 | 0.957 | 78.8 % |
| Group 6 | cell_32 | 3,358 | 26 | 1.210 | 0.946 | 78.2 % |
| Group 6 | cell_33 | 3,499 | 28 | 1.222 | 0.935 | 76.5 % |
| Group 6 | cell_34 | 3,558 | 28 | 1.215 | 0.936 | 77.0 % |
| Group 6 | cell_35 | 3,086 | 24 | 1.213 | 0.937 | 77.3 % |
| Group 6 | cell_36 | 3,651 | 28 | 1.210 | 0.944 | 78.0 % |
| Group 6 | cell_37 | 2,896 | 23 | 1.216 | 0.947 | 77.9 % |
| Group 7 | cell_38 | 3,965 | 47 | 1.214 | 0.952 | 78.4 % |
| Group 7 | cell_39 | 4,308 | 51 | 1.217 | 0.942 | 77.4 % |
| Group 7 | cell_40 | 3,968 | 47 | 1.214 | 0.942 | 77.6 % |
| Group 7 | cell_41 | 3,724 | 44 | 1.211 | 0.929 | 76.7 % |
| Group 7 | cell_42 | 3,673 | 44 | 1.218 | 0.945 | 77.6 % |
| Group 7 | cell_43 | 3,929 | 47 | 1.219 | 0.953 | 78.2 % |
| Group 8 | cell_44 | 3,517 | 28 | 1.214 | 0.929 | 76.5 % |
| Group 8 | cell_45 | 4,021 | 32 | 1.212 | 0.935 | 77.1 % |
| Group 8 | cell_46 | 3,571 | 28 | 1.212 | 0.958 | 79.1 % |
| Group 8 | cell_47 | 4,704 | 37 | 1.211 | 0.953 | 78.7 % |
| Group 8 | cell_48 | 3,497 | 28 | 1.210 | 0.948 | 78.4 % |
| Group 8 | cell_49 | 4,413 | 35 | 1.217 | 0.918 | 75.4 % |
| Group 9 | cell_50 | 3,761 | 56 | 1.223 | 0.957 | 78.3 % |
| Group 9 | cell_51 | 3,830 | 57 | 1.212 | 0.949 | 78.3 % |
| Group 9 | cell_52 | 3,891 | 58 | 1.215 | 0.956 | 78.7 % |
| Group 9 | cell_53 | 3,897 | 58 | 1.212 | 0.953 | 78.6 % |
| Group 9 | cell_54 | 3,910 | 58 | 1.208 | 0.957 | 79.2 % |
| Group 9 | cell_55 | 3,848 | 57 | 1.205 | 0.952 | 79.0 % |
| Group 10 | cell_56 | 6,091 | 68 | 1.213 | 0.954 | 78.6 % |
| Group 10 | cell_57 | 6,626 | 74 | 1.218 | 0.955 | 78.4 % |
| Group 10 | cell_58 | 6,612 | 73 | 1.208 | 0.953 | 78.9 % |
| Group 10 | cell_59 | 5,848 | 66 | 1.214 | 0.949 | 78.2 % |
| Group 10 | cell_60 | 7,156 | 77 | 1.208 | 0.956 | 79.1 % |
| Group 10 | cell_61 | 6,393 | 71 | 1.210 | 0.955 | 79.0 % |
| Group 11 | cell_62 | 3,002 | 33 | 1.211 | 0.946 | 78.1 % |
| Group 11 | cell_63 | 3,191 | 35 | 1.211 | 0.954 | 78.8 % |
| Group 11 | cell_64 | 3,124 | 34 | 1.206 | 0.939 | 77.8 % |
| Group 11 | cell_65 | 2,731 | 30 | 1.211 | 0.959 | 79.2 % |
Test programmes
- Group 1. 6 cells (cell_02 to cell_07), CyclingParameters.csv: charge 2C CC-CV, discharge 1.5C, depth of discharge 60 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 2. 6 cells (cell_08 to cell_13), CyclingParameters.csv: charge 2.417C CC-CV, discharge 1.5C, depth of discharge 60 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 3. 6 cells (cell_14 to cell_19), CyclingParameters.csv: charge 2C CC-CV, discharge 2C, depth of discharge 60 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 4. 6 cells (cell_20 to cell_25), CyclingParameters.csv: charge 2C CC-CV, discharge 1.5C, depth of discharge 80 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 5. 6 cells (cell_26 to cell_31), CyclingParameters.csv: charge 2.833C CC-CV, discharge 1.5C, depth of discharge 60 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 6. 6 cells (cell_32 to cell_37), CyclingParameters.csv: charge 2.417C CC-CV, discharge 2C, depth of discharge 60 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 7. 6 cells (cell_38 to cell_43), CyclingParameters.csv: charge 2.417C CC-CV, discharge 1.5C, depth of discharge 80 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 8. 6 cells (cell_44 to cell_49), CyclingParameters.csv: charge 3.25C CC-CV, discharge 1.5C, depth of discharge 60 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 9. 6 cells (cell_50 to cell_55), CyclingParameters.csv: charge 2C CC-CV, discharge 1.5C, depth of discharge 100 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 10. 6 cells (cell_56 to cell_61), CyclingParameters.csv: charge 2C CC-CV, discharge 2C, depth of discharge 80 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
- Group 11. 4 cells (cell_62 to cell_65), CyclingParameters.csv: charge 2.833C CC-CV, discharge 1.5C, depth of discharge 80 %; C-rates on the 1.2 Ah nominal capacity the README states. Drawn: reference capacity tests (about 0.40 A to 2.0 V), about every 3.5 days.
Columns of the CSV
The 1084 zip members (one cycling and one RPT series per cell, part files in numeric order, part0 and part00 both occur) were streamed with `unzip -p` (the cycling zips use Deflate64) through battery-data tools/convert_uconn_reil.py, Python standard library only, on Lemonergy's computer; nothing was unpacked to disk. The CRC-32 of every member was recomputed from the streamed bytes and matched the zip's central directory. Each source file entry gives the cell's cycling zip with its SHA-256 and, under members, every zip member the cell's rows come from (zip, member path, size and CRC-32 from the zip's directory): the members themselves have no SHA-256, the zips do. Cycles follow tools/cyclers.py exactly (noise floor 5 mA, a cycle = one charge followed by one discharge, |I| x dt over I > 0 and I < 0 with dt to the previous sample, the first sample of a cycle getting no interval, nothing integrated over an interval above 3600 s), on one time axis per cell; the per-cell results were interleaved with `convert_uconn_reil.py assemble`. Values are rounded as printed: Ah to 5 decimals, efficiency and volts to 4, seconds to 0.1.
| Column | Unit | Meaning |
|---|---|---|
batch | – | cycling group, CyclingParameters.csv 'Group Number' |
cell | – | cell_XX, the dataset's cell number |
cycle | – | row number per cell, 1-based, cycling and RPT rows in time order |
label | – | 'week W cycle N' (the files' Week Number and Cycle Number; several joined with ' + ' when a cycle spans protocols) or 'RPT n week W [reference capacity] k cycles since last RPT' |
charge_ah | Ah | charge integrated from current |
discharge_ah | Ah | discharge integrated from current |
charge_ah_reported | Ah | increments of the file's Capacity (Ah) counter on charging samples |
discharge_ah_reported | Ah | increments of the file's Capacity (Ah) counter on discharging samples |
coulombic_efficiency | – | discharge_ah / charge_ah (meaningless for partial and RPT rows, where charge and discharge do not start from the same state) |
v_max | V | highest voltage in the row's samples |
v_min | V | lowest voltage in the row's samples |
duration_s | s | length of the row's samples |
start_test_time_s | s | start on the cell's time axis, from the cell's first sample |
Data quality
No per-cell quality verdict was recorded for this dataset. Read the caveats below before comparing cells.
The manifest records these checks of the capacity integrated from current against the tester’s own counter, as differences in mAh:
| Rows compared | Count | Median (mAh) | 95th percentile (mAh) | Largest (mAh) |
|---|---|---|---|---|
| Cycling rows, discharge | 277,925 | 0.00 | 0.00 | 0.13 |
| Cycling rows, charge | 278,059 | 0.35 | 0.48 | 0.98 |
| Reference tests, discharge | 2,855 | 0.00 | 0.01 | 0.01 |
| Reference tests, charge | 2,855 | 0.14 | 0.15 | 0.15 |
Before comparing cells
- Ageing rows are partial cycles: each group cycles over a fixed depth of discharge (60, 80 or 100 %), so a cycling row's discharge_ah is that partial throughput, not the cell's capacity. The capacity measurements are the rows labelled '[reference capacity]', one per reference performance test (RPT): read capacity fade from them, as from XJTU's '[test capacity]' rows.
- An RPT row is not a whole RPT. Its charge_ah is the RPT's 'ref_chg' steps before the reference discharge (the charge from the 2.0 V cut-off to the 3.6 V CC-CV end, in four steps with the slow pulses between them not counted); its discharge_ah is the single 'ref_dchg' step (in this data about 0.40 A, to 2.0 V). v_max, v_min, start and duration cover those steps only; the duration spans the pulses between them. The RPT's later 'ref_chg' steps (recharging between fast pulses) and every pulse segment (slowpulse, fastpulse, ultrafastpulse) are not imported. Every RPT in the dataset has exactly one 'ref_dchg' step. The label carries the file's RPT Number, Week Number and Num Cycles (cycles since the previous RPT).
- Rows of a cell are its cycling and RPT rows in time order on one axis. The files' Time (s) restarts at each protocol (every half week) and each RPT; each is placed by its first Date stamp minus its Time. The stamps have 1 s resolution and no stated time zone; no protocol or RPT had to be moved to keep time increasing.
- Gaps: 1243 times a cycling protocol starts more than an hour after the previous one ended, with current flowing; these are where the RPTs and other stops fall, and nothing is integrated across them (cyclers' rule). No gap over an hour occurs inside a protocol.
- Cycles follow tools/cyclers.py: one charge followed by one discharge. A protocol that stops in mid-charge is completed by the next protocol's first charge, and cyclers counts that as one cycle: 1242 cycling rows carry two file cycles in their label (e.g. 'week 4.5 cycle 101 + week 5 cycle 1'). Their charge is two charges; in 364 of them it exceeds 1.5 x the 1.2 Ah nominal and is listed under exceptions.
- Integrated against the files' own Capacity (Ah) counter (which restarts at each step and counts up in both directions; its increments are attributed to charge or discharge by the sign of the current), over cycles where the reported value exceeds 0.05 Ah: cycling discharge median 0.0 mAh (max 0.13 mAh), cycling charge median 0.35 mAh (max 0.98 mAh), RPT discharge median 0.0 mAh, RPT charge median 0.14 mAh; 277925 and 2855 rows compared.
- Why charge is about 0.35 mAh below the counter: cyclers integrates each sample's current over the interval before it (right-rectangle). During the CV tail the current falls, so that rule under-counts; the tester's counter lies between right- and left-rectangle integration. Measured on cell_02 week 0 cycle 2: right 0.7777241 Ah, left 0.7783765 Ah, trapezoid 0.7780503 Ah, counter 0.7780188 Ah. Constant-current discharge shows no such difference. The values are left as cyclers computes them, so all datasets are integrated alike.
- The README says data are sampled at 1 Hz; the first samples of each step are 0.1 to 0.5 s apart, then about 1 s.
- Odd cycles kept as recorded: in cell_16, cell_48 the week 52 cycling file holds, under its 'cycle 1', a pulse and full-discharge sequence like an RPT, which cyclers splits into 10 rows with that same label.
- Spot-checked a second, independent way on the laptop (awk over unzip -p, grouped by the file's own Week and Cycle Number): cell_02 week 4.5 cycle 85 and week 5.5 cycle 28, cell_34 week 3 cycles 69 and 106 and week 4 cycle 21, cell_56 week 8 cycles 43 and 60 and week 8.5 cycle 88 agree with these rows to six decimals in charge and discharge, and exactly in v_max and v_min; for cell_02 'week 4.5 cycle 101 + week 5 cycle 1' the discharge agrees exactly and the charge is the two file cycles' charges together.
- Cell temperature is not in the files. The cells are 'LithiumWerks APR18650M1B' in the dataset; the product record's values come from the maker's data sheet, not from this dataset.
- Only the reference tests are drawn: the cycling rows are partial discharges at the group's depth of discharge, so their discharge_ah is throughput, not capacity. The capacity drawn is discharge_ah, integrated from current like the other datasets; for these rows it agrees with the tester's own counter (discharge_ah_reported) to 0.01 mAh at most. The horizontal axis is the cell's row number, which counts cycling and reference-test rows in time order.
Licence and how to cite
The values are published under CC BY 4.0, as the source is. Credit it as follows.
Cite: Nowacki, B., Ramamurthy, J., Thelen, A., Tischer, C., Pint, C. L., Hu, C. Rapid estimation of lithium-ion battery capacity and resistances from short duration current pulses. Journal of Power Sources 628, 235813 (2025). doi:10.1016/j.jpowsour.2024.235813
Credit: Data: Nowacki, B., Ramamurthy, J., Thelen, A., Tischer, C., Pint, C. L., Hu, C., UConn-ISU-ILCC LFP/Gr Battery Aging Dataset (UConn REIL), cited as J. Power Sources 628, 235813 (2025), doi:10.1016/j.jpowsour.2024.235813, CC BY 4.0. Per-cycle values computed by Lemonergy (battery-data).
Values pinned to battery-data revision e85dd43. The manifest names every source file by its SHA-256; the CSV’s own SHA-256 is 5b59a178ff4d72c5fc54735891003c31069a06e81a5f75ff4dd2d931cd7e2b75.
Related
- XJTU battery ageing data: 55 Lishen 18650 cells, cycle by cycle
- CALCE CS2 battery ageing data: 15 LiCoO2 cells, cycle by cycle
- Tongji/KIT NCA ageing data: 66 18650 cells, cycle by cycle
- Tongji/KIT NCM ageing data: 55 18650 cells, cycle by cycle
- Tongji/KIT NCM+NCA ageing data: 9 18650 cells at three discharge rates
- Michigan VTC6 data: 194 characterisations of 70 aged 18650 cells
- CMU eVTOL battery data: 22 VTC6 cells under aircraft missions
- NASA PCoE battery ageing data: 34 18650 cells, cycle by cycle
- Oxford battery degradation data: 8 Kokam pouch cells, test by test
- HYDRA ageing data: 32 LG MJ1 18650 cells under ship-like cycling
- REBELION ageing data: 160 Samsung 50E cells, four cycling strategies
- TEMPEST ageing data: a 280 Ah LFP cell over 700 cycles at 1C
- LiBforSecUse ageing data: 34 18650 NMC811 cells, 13 life-cycle tests
- VERSAPRINT cycle data: one Lishen 51 Ah cell, nine cycles
- EVERLASTING ageing data: 28 Samsung 35E cells under drive cycles
- FreeTwinEV module data: four Molicel P45B cells in parallel, 14 runs
- All open battery ageing data on Lemonergy
- How these datasets were imported and checked
- Find and compare battery cells