Open battery ageing data · Oxford 1
Oxford battery degradation data: 8 Kokam pouch cells, test by test
The Oxford Battery Degradation Dataset 1 (Howey and Birkl, University of Oxford, 2017) aged 8 Kokam SLPB533459H4 pouch cells of 740 mAh with an urban drive cycle at 40 °C. About every 100 drive cycles each cell was characterised: a 1C discharge and charge, and a slow pseudo-OCV discharge and charge. The file holds these tests only, not the drive cycles. Lemonergy computed one row per test pair from the file’s own charge counter. The values and the downloads are offered under the Open Database License, as the source is.
Download every test (CSV, 138 kB)Manifest (JSON): files, hashes, unitsLicence of the downloads (LICENSE.md)Chart and Excel downloadOriginal dataset
Free to download, no account needed. Or read it straight into Python:
import pandas as pd
cycles = pd.read_csv("https://lemonergy.com/data/ageing/oxford-2017/cycles.csv")- Cells
- 8 cells, pouch; maker: Kokam (Readme: 'Kokam CO LTD')
- Chemistry
- not stated
- Nominal capacity
- 0.74 Ah
- Tests
- 1,040, one row each
- Test programmes
- 1
- Published by
- University of Oxford
- Files retrieved
- 2026-11-12
Source: Oxford Battery Degradation Dataset 1 (8 x Kokam SLPB533459H4, 740 mAh), University of Oxford, doi:10.5287/bodleian:KO2kdmYGg. Licence: ODbL 1.0.
Cite: Howey, D., Birkl, C. Oxford Battery Degradation Dataset 1. University of Oxford (2017). doi:10.5287/bodleian:KO2kdmYGg. And, as the Readme asks: Birkl, C. R. Diagnosis and Prognosis of Degradation in Lithium-Ion Batteries. PhD thesis, Department of Engineering Science, University of Oxford (2017).
Notice: Contains information from the Oxford Battery Degradation Dataset 1 (Howey and Birkl, University of Oxford), which is made available under the Open Database License (ODbL), doi:10.5287/bodleian:KO2kdmYGg, https://opendatacommons.org/licenses/odbl/1-0/.
Licence and how to cite · Data quality · Every source file, by SHA-256
Capacity fade, test by test
1C discharge capacity of each characterisation, against the drive cycles run before it, one coloured line per cell. Point at a chart to read the values; download them as Excel.
The chart needs JavaScript; every cell’s values are in the table below and in the CSV.
Point at or touch a chart to read every cell’s value at that cycle. Drag across it with a mouse to zoom in. Click a line, or a cell’s name in the legend or table, to show that cell on its own; the others turn grey.Touch a chart to read the values at a cycle. Tap a cell’s name in the legend or the table to show it on its own; the others turn grey.
| Cell | Tests recorded | Points drawn | First (Ah) | Last (Ah) | Last / first |
|---|
Every cell
First and last discharge capacity of the tests the chart draws, for all 8 cells. Every row of every cell, with all its values, is in the CSV (138 kB).
| Programme | Cell | Tests recorded | Points drawn | First (Ah) | Last (Ah) | Last / first |
|---|---|---|---|---|---|---|
| drive-cycle-40C | Cell1 | 158 | 77 | 0.739 | 0.561 | 75.8 % |
| drive-cycle-40C | Cell2 | 146 | 73 | 0.735 | 0.545 | 74.2 % |
| drive-cycle-40C | Cell3 | 152 | 76 | 0.735 | 0.566 | 77.0 % |
| drive-cycle-40C | Cell4 | 94 | 47 | 0.734 | 0.581 | 79.2 % |
| drive-cycle-40C | Cell5 | 92 | 46 | 0.735 | 0.456 | 62.0 % |
| drive-cycle-40C | Cell6 | 92 | 46 | 0.733 | 0.579 | 79.0 % |
| drive-cycle-40C | Cell7 | 154 | 77 | 0.729 | 0.583 | 80.0 % |
| drive-cycle-40C | Cell8 | 152 | 76 | 0.728 | 0.559 | 76.8 % |
Test programmes
- drive-cycle-40C. All eight cells: the same drive-cycle ageing at 40 C, characterised about every 100 drive cycles (Readme). Drawn: 1C (740 mA) discharge of each characterisation, about every 100 drive cycles.
Columns of the CSV
Oxford_Battery_Degradation_Dataset_1.mat read with battery-data tools/convert_oxford_mat.py (in this repository; the method is open, as ODbL 4.6 asks). The file has no current column and holds only the characterisation tests, so nothing is integrated from current: a row's charge and discharge are the change of the file's own charge counter q over the test (mAh / 1000). One row per test pair in the order the tests ran: 1C (C1dc then C1ch) and pseudo-OCV (OCVdc then OCVch). t, a MATLAB date number, is converted to seconds; start_test_time_s counts from the cell's first sample. A test array holding two recordings (stop over one hour, counter restarting) becomes one row per recording. Values are rounded as printed: Ah to 5 decimals, efficiency and volts to 4, seconds to 0.1. tools/cyclers.py cannot read .mat and its integration rule does not apply to a file without current.
| Column | Unit | Meaning |
|---|---|---|
batch | – | one batch: all cells aged the same way (drive-cycle-40C) |
cell | – | the file's struct name, Cell1 to Cell8 |
cycle | – | row number within the cell, 1-based (not a drive-cycle count) |
label | – | the test name (cycNNNN: after NNNN drive cycles), which pair of tests, [characterisation], and any note on the recording |
charge_ah | Ah | change of the file's charge counter q over the charge test (C1ch or OCVch) |
discharge_ah | Ah | change of the file's charge counter q over the discharge test (C1dc or OCVdc), as a positive number |
charge_ah_reported | Ah | blank: the file has no summary figure apart from the counter used in charge_ah |
discharge_ah_reported | Ah | blank: as charge_ah_reported |
coulombic_efficiency | – | discharge_ah / charge_ah (the discharge comes before the charge) |
v_max | V | highest voltage in the two tests |
v_min | V | lowest voltage in the two tests |
duration_s | s | from the start of the discharge to the end of the charge, rest between them included |
start_test_time_s | s | start of the row, seconds after the cell's first sample (cyc0000 C1dc) |
Data quality
Overall: Good for the capacity fade of one small Kokam pouch cell under drive-cycle ageing at 40 C, at 1C and near equilibrium, over 5,000 to 8,200 cycles, and for pseudo-OCV curves once you go back to the raw file. Do not use it for drive-cycle behaviour (not in the file), for internal resistance (no current), or as eight independent cells without dropping Cell1's repeated rows and reading the per-cell caveats.
8 cells checked: 5 usable, 3 usable with caveats, 0 not usable.
| Cell | Verdict | Why |
|---|---|---|
| Cell1 | usable with caveats | Four recordings repeated in the file: cyc7100 is a sample-for-sample copy of cyc7000 (the real cyc7100 test is missing), and the cyc3200 and cyc4500 pseudo-OCV arrays each hold their own recording plus a copy of the next test's (cyc3300, cyc4600). cyc1600 has a constant 0.5 C temperature (sensor not recorded). All kept and labelled. |
| Cell2 | usable with caveats | cyc7400 is 10 % lower at 1C (discharge and charge) and recovers at cyc7500; pseudo-OCV coulombic efficiency 0.943 there. Kept as recorded. |
| Cell3 | usable | cyc3300 is missing as well as the five tests missing for every cell. |
| Cell4 | usable | No finding beyond those common to all cells. |
| Cell5 | usable with caveats | The last test, cyc5000, is 25 % (1C) and 16 % (pseudo-OCV) below cyc4800, with a pseudo-OCV coulombic efficiency of 0.926: either the cell failed or the test is bad; the dataset does not say. |
| Cell6 | usable | No finding beyond those common to all cells. |
| Cell7 | usable | No finding beyond those common to all cells. |
| Cell8 | usable | cyc0200 is missing as well as the five tests missing for every cell. |
Before comparing cells
- Characterisation, not ageing cycles: each row is one characterisation test pair taken after about 100 drive cycles more; the drive cycles themselves are not in the file. The test's own name (cycNNNN, the number of drive cycles before it) is at the start of the label.
- Capacities are the file's own charge counter: the file has no current, so no integrated-versus-counter check is possible. The one file with current, ExampleDC_C1.mat (not imported), shows the tester's counter agrees with its current to 0.03 mAh.
- Coulombic efficiency of the 1C rows is 1.02 to 1.08 and grows with age. It is not a fault: the 1C discharge starts from the full CC-CV charge of the ageing protocol, and the 1C charge recorded after it is constant current only, stopping at 4.2 V. Use the pseudo-OCV rows (median 0.997) for efficiency.
- The discharge comes first in every test pair; a row's coulombic efficiency is that discharge over the charge that follows it.
- Cell1 repeats four recordings, labelled '[same samples as ...]': cyc7100 is a copy of cyc7000 (the real cyc7100 is missing), and the cyc3200 and cyc4500 pseudo-OCV arrays each hold a second recording identical to the next test's (cyc3300, cyc4600). These rows are kept, so Cell1's start times run backwards three times. Drop one of each pair before fitting a fade curve.
- Missing tests: cyc1500, 1700, 3400, 4700 and 4900 for every cell; cyc3300 for Cell3; cyc0200 for Cell8.
- Temperature: the pseudo-OCV tests of cyc3500 (charge) and cyc3700 (both) ran at 22 to 26 C, not 40 C, for all cells. Cell1 cyc1600 records a constant 0.5 C (sensor not recorded).
- Cell5's last test (cyc5000) is 25 % lower at 1C than cyc4800; Cell2's cyc7400 is 10 % lower and recovers at cyc7500. Kept as recorded.
- The Readme says t is in seconds; it is a MATLAB date number in days. The chemistry is not stated by the source and is not filed.
- Cell1 holds repeated recordings: cyc7100 is a copy of cyc7000 (the real cyc7100 is missing), so it is drawn once, at cyc7000. Both rows stay in the CSV.
Licence and how to cite
The values and the downloads here are offered under ODbL 1.0, as the source is (individual contents: DbCL 1.0), not under CC BY. If you publicly use a database made from them, it must be under the ODbL too. The licence file travels with the downloads: LICENSE.md. Credit it as follows.
Notice: Contains information from the Oxford Battery Degradation Dataset 1 (Howey and Birkl, University of Oxford), which is made available under the Open Database License (ODbL), doi:10.5287/bodleian:KO2kdmYGg, https://opendatacommons.org/licenses/odbl/1-0/.
Cite: Howey, D., Birkl, C. Oxford Battery Degradation Dataset 1. University of Oxford (2017). doi:10.5287/bodleian:KO2kdmYGg. And, as the Readme asks: Birkl, C. R. Diagnosis and Prognosis of Degradation in Lithium-Ion Batteries. PhD thesis, Department of Engineering Science, University of Oxford (2017).
Credit: Contains information from the Oxford Battery Degradation Dataset 1 (Birkl and Howey, University of Oxford, doi:10.5287/bodleian:KO2kdmYGg), which is made available here under the Open Database License (ODbL) 1.0, https://opendatacommons.org/licenses/odbl/1-0/. Per-test values computed by Lemonergy (battery-data) and offered under the same licence.
Values pinned to battery-data revision e85dd43. The manifest names every source file by its SHA-256; the CSV’s own SHA-256 is 721ee7b395e37c1453a88872debc7d5a7eea6de4a9c265fc8084e05883e572d2.
Related
- XJTU battery ageing data: 55 Lishen 18650 cells, cycle by cycle
- CALCE CS2 battery ageing data: 15 LiCoO2 cells, cycle by cycle
- Tongji/KIT NCA ageing data: 66 18650 cells, cycle by cycle
- Tongji/KIT NCM ageing data: 55 18650 cells, cycle by cycle
- Tongji/KIT NCM+NCA ageing data: 9 18650 cells at three discharge rates
- Michigan VTC6 data: 194 characterisations of 70 aged 18650 cells
- CMU eVTOL battery data: 22 VTC6 cells under aircraft missions
- NASA PCoE battery ageing data: 34 18650 cells, cycle by cycle
- UConn LFP ageing data: 64 18650 cells under 11 cycling conditions
- HYDRA ageing data: 32 LG MJ1 18650 cells under ship-like cycling
- REBELION ageing data: 160 Samsung 50E cells, four cycling strategies
- TEMPEST ageing data: a 280 Ah LFP cell over 700 cycles at 1C
- LiBforSecUse ageing data: 34 18650 NMC811 cells, 13 life-cycle tests
- VERSAPRINT cycle data: one Lishen 51 Ah cell, nine cycles
- EVERLASTING ageing data: 28 Samsung 35E cells under drive cycles
- FreeTwinEV module data: four Molicel P45B cells in parallel, 14 runs
- All open battery ageing data on Lemonergy
- How these datasets were imported and checked
- Find and compare battery cells